Aluminium powder coating
Powder coating of aluminium
We chemically pre-treat aluminium profiles, sheets, castings and facade elements in a six-stage immersion line prior to powder coating.
Aluminium requires a different pre-treatment process from steel. Instead of abrasive blasting, we use chemical immersion: an acid degreasing and etching bath, two rinses, zirconium passivation, a further rinse and a final rinse in demineralised water. Bath concentrations and pH levels are monitored regularly.
Zirconium passivation forms a thin nanoceramic conversion layer on the aluminium surface, significantly improving paint adhesion and resistance to filiform and underfilm corrosion.
Aluminium pre-treatment
Six treatment baths before coating
We pre-treat aluminium chemically by immersion: acid degreasing and etching, rinsing, zirconium passivation and a final rinse in demineralised water. We closely monitor the parameters of every bath.
-
- Product
- Alfideox 83
- Temperature
- 30–35 °C
- Time
- 5–15 min
- Parameters and control
- Acid bath, concentration controlled by titration. Working concentration min. 20 g/l (2%).
-
- Product
- Mains water
- Temperature
- ambient
- Time
- 1–2 min
-
- Product
- Mains water
- Temperature
- ambient
- Time
- 1–2 min
-
- Product
- Ferropas 7815
- Temperature
- ambient
- Time
- 0.5–2 min
- Parameters and control
- Concentration and pH control. Working concentration min. 3–4 g/l (0.3–0.4%), bath pH 3–4.
-
- Product
- Mains water
- Temperature
- ambient
- Time
- 1–2 min
-
- Product
- DEMI water
- Temperature
- ambient
- Time
- 1–2 min
- Parameters and control
- Conductivity max. 30 µS/cm.
How we work
Six steps to a durable finish
-
We agree on the colour, finish, quantity and lead time. Collection and delivery are available on request.
-
Steel is shot blasted to Sa 2–Sa 3; aluminium undergoes a six-stage immersion process with zirconium passivation.
-
An electrostatic spray gun applies charged powder particles to the earthed workpiece — reaching corners and recesses evenly.
-
Inside the curing oven at 150 to 230 °C, the powder melts and cross-links into a uniform, durable coating.
-
We inspect surface appearance, coating thickness and adhesion — using the EN ISO 2409 cross-cut test.
-
Finished parts are packed for collection or delivered directly to your address.